陰離子(zi)交換(huan)樹(shu)(shu)脂,陽離子(zi)樹(shu)(shu)脂技術文章
陰離子交換樹脂,陽離子樹脂技術文章 專(zhuan)業生(sheng)產:陰陽離(li)子交(jiao)換(huan)樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 大孔吸(xi)附樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 軟化水(shui)樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 混床MB樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 18兆歐超純水(shui)拋(pao)光樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 線切(qie)割慢走絲樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 污水(shui)脫(tuo)色樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 電鍍廢水(shui)除(chu)鎳除(chu)鉻(ge)樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 除(chu)鐵、除(chu)銅、除(chu)磷、除(chu)硼、除(chu)坲除(chu)重金屬樹(shu)(shu)(shu)(shu)(shu)脂(zhi),酸(suan)回收樹(shu)(shu)(shu)(shu)(shu)脂(zhi),鰲(ao)合樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 食品(pin)級樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 提礬樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 吸(xi)金樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 提銀樹(shu)(shu)(shu)(shu)(shu)脂(zhi) 強(qiang)酸(suan)強(qiang)堿弱酸(suan)弱堿四(si)大類幾(ji)十種型號(hao)有:001×7、001×8、732、717、201×7、201×4、D001、D201、D301、D113、D101、H103、D403、D408等
產品(pin)名稱: | 201×7(717)強堿性苯乙烯系陰離子交換樹脂 | |
產品(pin)圖: |
| |
產品簡介: | 201×7是在交聯為7%的苯(ben)乙烯-二乙(yi)烯苯共(gong)聚體上(shang)帶(dai)有季銨(an)基(ji)[-N(CH3)3OH]的陰離子交換樹脂。主要用(yong)于純(chun)水(shui)(shui)制備、廢水(shui)(shui)處理、生化(hua)制品(pin)及濕法冶金中鎢、鉬(mu)的提(ti)取。 | |
理化(hua)性能指標: | 指標名稱 | 指標 |
執行標準: | GB/T13660-92 | |
外(wai)觀 : | 半透明球狀顆粒(li) | |
出廠型式 : | CLˉ | |
含水量 % : | 42.00-48.00 | |
質量全(quan)交(jiao)換(huan)容量 mmol/g : | ≥3.60 | |
體積(ji)全交換(huan)容(rong)量 mmol/ml : | ≥1.35 | |
濕視密度 g/ml : | 0.67-0.73 | |
濕(shi)真密度 g/ml : | 1.060-1.100 | |
范圍粒度 % : | (0.315-1.25mm)≥95 | |
下限粒度 % : | (<0.315mm)≤1 | |
有效(xiao)粒徑 mm : | 0.400-0.700 | |
均(jun)一系數 : | ≤1.60 | |
磨后圓球率 %: | ≥90 | |
使用參考指標: | 指標名稱(cheng) | 指標 |
pH范圍 | 1-14 | |
使用溫度(du)°C | OHˉ:40 CLˉ:100 | |
轉型膨(peng)脹率(CLˉ→OHˉ)% | ≤27 | |
工(gong)作交換(huan)容量 mmol/L | ≥450 | |
運行流速 m/h | 15-30 |
陰、陽離子交換樹脂樹脂的貯存(cun):
離子(zi)交換樹(shu)脂肪內(nei)含有一定(ding)量(liang)的水(shui)份,在(zai)(zai)運(yun)輸及貯存(cun)過程中(zhong)應(ying)(ying)盡量(liang)保持這(zhe)部(bu)分水(shui)。如貯存(cun)過程中(zhong)樹(shu)脂脫了水(shui),應(ying)(ying)先(xian)用濃食鹽水(shui)(-10%)浸(jin)泡,再(zai)逐漸稀釋,不(bu)得直接放于水(shui)中(zhong),以免樹(shu)脂急劇(ju)膨脹而破碎(sui)。在(zai)(zai)長(chang)期貯存(cun)中(zhong),強型(xing)(xing)樹(shu)脂應(ying)(ying)轉變成鹽型(xing)(xing),弱(ruo)型(xing)(xing)樹(shu)脂可(ke)(ke)轉變成相應(ying)(ying)的氫型(xing)(xing)或游離堿型(xing)(xing)也可(ke)(ke)轉為鹽型(xing)(xing),然后浸(jin)泡在(zai)(zai)潔凈的水(shui)中(zhong)。樹(shu)脂在(zai)(zai)貯存(cun)或運(yun)輸過程中(zhong),應(ying)(ying)保持在(zai)(zai)5-40°C的溫度環境中(zhong),避免過冷或過熱,影(ying)響(xiang)質量(liang)。若冬季(ji)沒有保溫設備(bei)時,可(ke)(ke)將(jiang)樹(shu)脂貯存(cun)在(zai)(zai)食鹽水(shui)中(zhong),食鹽水(shui)的溫度可(ke)(ke)根(gen)據氣溫而定(ding)。
新樹脂(zhi)的預處(chu)理:
新樹(shu)脂(zhi)常含有溶(rong)劑、未參加聚合反應的物質(zhi)(zhi)和少量(liang)低聚合物,還可能(neng)吸(xi)著鐵、鋁、銅等重金屬離(li)子。當樹(shu)脂(zhi)與水(shui)(shui)、酸、堿或其(qi)他溶(rong)液相接觸(chu)時,上述可溶(rong)性雜質(zhi)(zhi)就(jiu)會轉入溶(rong)液中,在(zai)(zai)使用初期污染出水(shui)(shui)水(shui)(shui)質(zhi)(zhi)。所以,新樹(shu)脂(zhi)在(zai)(zai)投運(yun)前要進行預處(chu)理。
陽(yang)樹脂的預(yu)處理
陽樹脂(zhi)預處理步驟如下:
首先使用(yong)飽(bao)和食鹽水(shui)(shui),取其(qi)(qi)量約等于(yu)被處理樹(shu)脂體積的兩倍,將樹(shu)脂置于(yu)食鹽溶液中浸(jin)泡18-20小(xiao)時,然后放盡(jin)食鹽水(shui)(shui),用(yong)清水(shui)(shui)漂洗(xi)(xi)(xi)凈(jing),使排出(chu)水(shui)(shui)不帶黃色;其(qi)(qi)次再用(yong)2%-4%NaOH溶液,其(qi)(qi)量與(yu)上相同,在其(qi)(qi)中浸(jin)泡2-4小(xiao)時(或作(zuo)小(xiao)流量清洗(xi)(xi)(xi)),放盡(jin)堿液后,沖洗(xi)(xi)(xi)樹(shu)脂直至排出(chu)水(shui)(shui)接近(jin)中性為止。后用(yong)5%HCL溶液,其(qi)(qi)量亦與(yu)上述相同,浸(jin)泡4-8小(xiao)時,放盡(jin)酸(suan)液,用(yong)清水漂流至中性(xing)待用。
陰(yin)離(li)子交換樹(shu)脂
樹(shu)脂的貯存(cun):
離子(zi)交換樹(shu)脂(zhi)肪內(nei)含有一定(ding)量(liang)的水(shui)(shui)份,在(zai)(zai)運輸及(ji)貯存過(guo)(guo)程中(zhong)(zhong)應(ying)(ying)(ying)(ying)盡量(liang)保持(chi)這部分水(shui)(shui)。如貯存過(guo)(guo)程中(zhong)(zhong)樹(shu)脂(zhi)脫了水(shui)(shui),應(ying)(ying)(ying)(ying)先用濃食鹽水(shui)(shui)(-10%)浸泡,再逐(zhu)漸(jian)稀(xi)釋,不(bu)得直接放于水(shui)(shui)中(zhong)(zhong),以免(mian)樹(shu)脂(zhi)急劇(ju)膨脹而破碎。在(zai)(zai)長(chang)期貯存中(zhong)(zhong),強型(xing)(xing)樹(shu)脂(zhi)應(ying)(ying)(ying)(ying)轉(zhuan)變成鹽型(xing)(xing),弱型(xing)(xing)樹(shu)脂(zhi)可轉(zhuan)變成相(xiang)應(ying)(ying)(ying)(ying)的氫型(xing)(xing)或游離堿型(xing)(xing)也可轉(zhuan)為鹽型(xing)(xing),然后浸泡在(zai)(zai)潔凈的水(shui)(shui)中(zhong)(zhong)。樹(shu)脂(zhi)在(zai)(zai)貯存或運輸過(guo)(guo)程中(zhong)(zhong),應(ying)(ying)(ying)(ying)保持(chi)在(zai)(zai)5-40°C的溫度環境(jing)中(zhong)(zhong),避免(mian)過(guo)(guo)冷或過(guo)(guo)熱,影(ying)響質量(liang)。若(ruo)冬季沒有保溫設備(bei)時,可將樹(shu)脂(zhi)貯存在(zai)(zai)食鹽水(shui)(shui)中(zhong)(zhong),食鹽水(shui)(shui)的溫度可根(gen)據氣(qi)溫而定(ding)。
新樹脂的(de)預處理:
新(xin)樹(shu)脂常(chang)含有(you)溶(rong)劑(ji)、未參加聚(ju)(ju)合反應的物質和少量低(di)聚(ju)(ju)合物,還可能(neng)吸(xi)著(zhu)鐵、鋁、銅等重(zhong)金屬離子。當(dang)樹(shu)脂與水(shui)、酸、堿或(huo)其他溶(rong)液(ye)相接觸時,上述可溶(rong)性雜質就會(hui)轉入溶(rong)液(ye)中(zhong),在使用(yong)初期污染出水(shui)水(shui)質。所以,新(xin)樹(shu)脂在投運前(qian)要進行(xing)預處理。
陰樹脂的(de)預處理
其預處理方法中的步與陽樹脂預處理方法中的步相同;而后用5%HCL浸泡4-8小時,然后放盡酸液,用水清洗至中性;而后用2%-4%NaOH溶液浸泡4-8小時后,放盡堿(jian)液,用清水(shui)洗(xi)至(zhi)中(zhong)性(xing)待(dai)用。
陰離子交換樹脂,陽離子樹脂技術文章
新購樹脂常殘存較多有機溶劑,低分子聚合物及有機雜質,運用前有必要盡量除掉,否則將影響樹脂的運用壽命。
1.將樹脂放在一大桶內,先用清水漂洗潔凈,濾干。
2.用80%~90%工業乙醇浸泡24小時,洗去樹脂內的乙醇溶性有機物然后抽干(濾液供收回乙醇)。
3.用40~50℃的熱水浸泡2小時,洗滌幾回后,再浮選或篩選出粒度適宜的樹脂。意圖是洗去樹脂內的水溶性雜質和乙醇味。然后抽干。
4.用4倍于樹脂量的2摩爾/升鹽酸(1:5)溶液浸泡處理2小時(要常常翻動),意圖是洗去酸溶性雜質。用蒸餾水或自來水洗至中性,抽干。
5.用4倍于樹脂量的2摩爾/升(8%)氫氧化鈉溶液浸泡2小時(需常常翻動),意圖是洗去堿溶性雜物。用蒸餾水或自來水洗至中性,抽干,備用。
6.如果是陰離子樹脂,可轉型為C1型或OH型,用鹽酸按上法處理一次即可;如是陽離子樹脂,可轉為H型或Na型,用氫氧化鈉按上法處理一次即可。
再生,用過的樹脂。如期望陽離子樹脂為H型、Na型或NH4型,則可別離用鹽酸、氫氧化鈉或氫氧化銨處理;要使陰離子樹脂為C1型、OH型,則可用鹽酸或氫氧化鈉別離處理。
樹脂宜保存于陰涼處,但不宜深凍,因深凍會損壞樹脂的內部結構。短期寄存可置于1摩爾/升鹽酸或氫氧化鈉溶液中。長時間寄存可參加適量防腐劑封存。遇到樹脂長霉,可用1%甲醛浸泡1小時后,再漂洗潔凈,然后進行再行處理。